Vacuum forming mold design guide

Draft Angles and Radii for Vacuum Forming

Draft lets the part come off the mold. Radii keep the plastic from thinning out in the corners. Get both right and most release and thinning problems go away.

Male mold (plug)Female mold (cavity) draft Part shrinks onto it: needs more draft Part shrinks away from it: needs less

Why male molds need more draft

As the formed part cools it shrinks. On a male mold (a plug the sheet drapes over) the part shrinks onto the mold and grips it, so it needs more draft to release. On a female mold (a cavity) the part shrinks away from the walls, so it can get by with less.

Typical starting points

These are common starting points, not hard rules. Textured surfaces, deep draws and high-shrink materials such as polypropylene and polyethylene all call for more draft.

  • Female molds: often about 1° to 3°
  • Male molds: often about 3° to 5° or more
  • Add draft for textured surfaces and deep walls
  • More draft is always easier to form than less

Corner radii

Sharp corners are where plastic stretches thinnest and where formed parts crack. As a rule of thumb, make inside radii at least equal to the sheet thickness, and larger where you can. Generous radii on a female mold's bottom corners and on a male mold's top edges make the biggest difference.

Undercuts

An undercut is any feature that would lock the part onto the mold. Small undercuts can sometimes pop off flexible materials. Larger ones need loose inserts, slides or a split mold, so design them in on purpose.

Written by Shaun Butler, a mechanical design engineer who has machined thermoforming molds, master tooling and plug assists for packaging and medical customers for many years, and a former lead engineer and VP of Operations at Count Machinery.

Need a mold made?

Prototype molds in days, aluminum production molds in about 1–2 weeks.